A galvanised grating lasts decades in urban air but only years by the sea or in a swimming pool. Here is how long which material lasts where – with the figures from DIN EN ISO 1461 and 14713 instead of gut feeling.
1. Hot-dip galvanising to DIN EN ISO 1461 – the standard
All custom gratings are fully hot-dip galvanised after pressing and banding: degreasing, pickling, flux, immersion in molten zinc at approx. 450 °C. This does not create an applied layer but an iron-zinc alloy bonded to the steel – which is why zinc does not flake off like paint. DIN EN ISO 1461 specifies the minimum coating thicknesses:
| Steel thickness | local min. | mean min. | On the grating |
|---|---|---|---|
| 1.5 – 3 mm | 45 µm | 55 µm | Bearing bars 2 mm, cross bars |
| > 3 – 6 mm | 55 µm | 70 µm | Bearing bars 3–5 mm, edge banding |
| > 6 mm | 70 µm | 85 µm | Frame angles, stair tread end plates |
Zinc protects in two ways: as a barrier and cathodically – at scratches and cut edges up to approx. 1–2 mm wide, the surrounding zinc sacrifices itself and the steel does not rust. That is what sets hot-dip galvanising apart from any coating.
2. Service life by environment (DIN EN ISO 14713-1 / ISO 9223)
| Category | Environment | Zinc loss / year | Protection period at 55–70 µm |
|---|---|---|---|
| C2 | Rural, dry interiors | 0.1 – 0.7 µm | > 50 years |
| C3 | Urban, suburban, light industry, damp rooms | 0.7 – 2.1 µm | 30 – 50+ years |
| C4 | Industrial, coastal (without salt spray), swimming pool surroundings | 2.1 – 4.2 µm | 15 – 30 years |
| C5 | Coastal with salt spray, chemical, de-icing salt splash | 4.2 – 8.4 µm | 8 – 15 years → stainless steel or duplex |
What matters is not the postcode but the micro-location: a light well under the roof overhang is C3; the channel grating by the road that gets de-icing salt splash every winter is C5. There, zinc at the splash line corrodes through in 5–10 years, while the same grating in the garden lasts 50 years.
3. Stainless steel: 304 (V2A) or 316 (V4A)?
| V2A / 304 (1.4301 / 1.4307) | V4A / 316 (1.4571 / 1.4404) | |
|---|---|---|
| Alloy | Cr-Ni | Cr-Ni-Mo (2–2.5 % molybdenum) |
| Resistant to | Water, urban air, food, cleaning agents | Chlorides as well: de-icing salt, sea water, pool water |
| Surface rust / pitting | possible with salt | much more resistant |
| Typical | House entrance, terrace, kitchen, façade inland | Swimming pool, coast, ramps and car parks with de-icing salt, chemicals |
| Price compared with galvanised | approx. 2 – 3× | approx. 2.5 – 3.5× |
Stainless steel gratings are pickled (matt silver, heat tint at the welds removed) or, on request, electropolished (smoother, more hygienic, brighter – swimming pools, food). Important: never work stainless steel with steel tools or store it wet against galvanised material for long periods – embedded iron particles cause surface rust, which is often mistaken for “rusting stainless steel”.
4. Powder coating and the duplex system
Powder coating alone on steel is unsuitable for gratings – every edge rusts underneath. What makes sense is the duplex system: hot-dip galvanised + powder-coated. Zinc protects cathodically, the powder layer (60–120 µm, any RAL colour) protects the zinc from wear; according to DIN EN ISO 14713-1, the protection period rises to 1.5 to 2.3 times the sum of the individual layers. Typical for façades, balconies, visible gratings, house surrounds in anthracite (RAL 7016) and stair treads. Note: coated gratings are somewhat smoother (check slip resistance) and should not be cut on site. Powder coating for custom gratings on request, standard products under powder coating for gratings.
5. GRP and aluminium as alternatives
| Criterion | Steel, galvanised | Stainless steel 316 | GRP | Aluminium |
|---|---|---|---|---|
| Corrosion | good, not with salt/chlorine | very good | very good (chemicals, wastewater plants) | good, not with alkalis |
| Load capacity / stiffness | very high | very high | medium, large deflection | medium |
| Weight | base | as steel | approx. 50 % | approx. 35 % |
| Electrically conductive | yes | yes | no (advantage for electrical, rail) | yes |
| Fire behaviour | A1 non-combustible | A1 | combustible (flame-retardant possible) | A1, melts at 660 °C |
| UV / ageing | – | – | surface chalks, sand wears it | – |
| Price | base | 2.5–3.5× | 1.5–2× | 2–3× |
GRP gratings and accessories are available from FeNau GRP; aluminium mainly as jetty gratings.
6. The most common mistakes in practice
- White rust: white, powdery spots on freshly galvanised gratings stored wet without air circulation (plastic sheeting, stacks). Not a defect – brush off when dry and it disappears. Store gratings ventilated, at an angle and with spacers.
- Cutting on site: a cut destroys the zinc layer; touch up the edge twice with zinc-rich paint (≥ 90 % Zn). Better: order to size.
- Galvanic corrosion: galvanised on a stainless steel or aluminium frame is not critical when dry; under constant wet conditions, separate with EPDM tape. Galvanised grating on copper sheet (gutter, downpipe): always separate.
- Welding on a galvanised grating: only with fume extraction (zinc oxide fumes, “metal fume fever”) and touching up afterwards.
- De-icing salt: do not spread salt on galvanised gratings in winter – use grit or sand and rinse off in spring.
Questions and answers
How long does a hot-dip galvanised grating last?
In urban and rural air (C2–C3), 30–50 years and longer without maintenance; in industrial or coastal air (C4), 15–30 years; with de-icing salt splash or chlorine (C5), only 8–15 years – choose 316 stainless steel there.
How thick is the zinc layer?
Under DIN EN ISO 1461, at least 45 µm local / 55 µm mean for 1.5–3 mm steel and 55 / 70 µm for 3–6 mm steel thickness.
304 or 316 – which do I need?
304 (1.4301) for entrances, terraces and façades inland; 316 (1.4571/1.4404) wherever there are chlorides: swimming pools, coast, de-icing salt, chemicals.
Can I get a grating in a RAL colour?
Yes, as a duplex system: hot-dip galvanised and then powder-coated in any RAL colour – on request for custom gratings, standard products in the FeNau shop.
What are the white spots on my new grating?